Permeable interlocking pavers (PICP)
Permeable interlocking concrete pavement, or PICP, lets rain pass through open joints in the paver surface into a layer of clean stone underneath, instead of running off. It is built differently from a regular paver patio, from the joint material down to the way the soil is treated.
How PICP works
The Concrete Masonry and Hardscapes Association (CMHA, which now includes ICPI) describes PICP as a pavement system that lets stormwater infiltrate through the surface into an underlying stone reservoir, and classes it as a stormwater best management practice and low-impact development tool. The pavers are solid concrete units with molded joints or openings, and they must meet ASTM C936. The water goes through the joints, not through the pavers. For a short definition, see the glossary entry on permeable pavers.
The layers, top to bottom
| Layer | What CMHA specifies |
|---|---|
| Pavers | ASTM C936 units; at least 3 1/8 in. (80 mm) thick for vehicle areas, 2 3/8 in. (60 mm) allowed for pedestrian areas |
| Joint stone | Angular ASTM No. 8, No. 89 or No. 9 stone, filled to within 1/4 in. (6 mm) of the surface; unit spacing 1/2 in. (12 mm) or less to meet ADA requirements |
| Bedding course | Open-graded crushed stone, typically 2 in. (50 mm) of ASTM No. 8, not sand |
| Base reservoir | Typically 4 in. (100 mm) of ASTM No. 57 stone; at least 6 in. (150 mm) for pedestrian applications |
| Subbase reservoir | Larger 3 to 2 in. stone (ASTM No. 2, 3 or 4), thickness set by water storage and traffic; may be omitted for pedestrian or residential driveway use, with a thicker base instead |
| Underdrain | Perforated pipe where the soil drains slowly |
| Geotextile | Specified by the designer to separate the subbase from the soil |
Compare this with the standard build: a standard paver patio uses concrete sand for bedding and fine sand in the joints, as in the concrete paver specification. A permeable system swaps both for open-graded stone, so that water can pass through.
The soil underneath
CMHA says the subgrade is generally not compacted, because compaction substantially reduces infiltration. How fast the soil takes water determines how much drains out of the stone layer into the ground. Where soils drain poorly, designers add underdrains, and some clays are compacted for stability, in which case the design has to allow for the lower infiltration. This is an engineering decision. If the site is near a foundation, slopes toward a house or has clay or high groundwater, have a design professional size the reservoir.
Edges
Curbs of cast-in-place, precast or cut stone are typically at least 9 in. (225 mm) high and sit on the compacted No. 2 subbase. Pedestrian areas and residential driveways may instead use compacted dense-graded berms with plastic or metal edging secured with steel spikes. A general overview of edging is on how to install paver edge restraints.
Maintenance and when it needs cleaning
PICP needs regular upkeep to keep the joints open. CMHA’s maintenance guide gives these routine and trigger points:
- Weekly: broom or blow off debris; clear debris after severe storms.
- Twice a year: remove debris after fall leaf drop and after winter snow, and top up joint stone to the bottom of the paver chamfers.
- Joints often need refilling 3 to 6 months after installation because the stone settles.
- Ponding over more than 20% of the surface calls for cleaning, and standing water for more than 15 minutes during or after a storm suggests the surface is nearing clogging.
- Surface infiltration is tested to ASTM C1701, with a recommended minimum of 100 in./hr for a new surface. A ponded-area rate consistently below 20 in./hr needs immediate cleaning.
Winter care
For snow, CMHA prefers hard rubber blades over steel and suggests confirming in writing that a commercial plow operator uses protective edges. It lists sodium, calcium and potassium chloride as acceptable deicers used sparingly, and says to avoid magnesium chloride and anti-icers containing ammonium nitrate or ammonium sulfate. Winter sand is not recommended; if it is used, vacuum it out in spring. Jointing stone is the preferred traction alternative. See also ice melt and paver warranties.
Related
All hardscape materials · Concrete pavers explained · Pavers and patios guide
FAQ
Does water drain through the pavers themselves?
No. The pavers are solid units. Water passes through the open joints, which are filled with small angular stone, and into the stone reservoir below.
Can I use regular polymeric sand in permeable pavers?
No. CMHA specifies angular ASTM No. 8, 89 or 9 stone in the joints and an open-graded stone bedding course, not sand.
How thick are the layers under permeable pavers?
Typically 2 in. of No. 8 bedding stone and 4 in. of No. 57 base, with a thicker subbase of larger stone where water storage or traffic requires it. Pedestrian areas need at least 6 in. of base.
How do I know when permeable pavers are clogged?
CMHA lists warning signs: ponding over more than 20% of the surface, or standing water lasting more than 15 minutes during or after rain.
Planning information only, not engineering advice. Permeable pavement is a designed system; layer thicknesses depend on soil and load, and local stormwater rules may apply. Sources checked Nov 23, 2026.