Concrete dusting and crazing

Two surface problems get confused: dusting, where a hardened slab turns to loose powder, and crazing, where a network of hairline cracks appears. Both trace back to what happened to the top layer during finishing and curing. The National Ready Mixed Concrete Association (NRMCA) covers each in its Concrete in Practice series.

How to tell them apart

DustingCrazing
What you seePowder or chalk on the surface that comes off on shoes or a broom.Fine, random cracks forming irregular hexagonal patches, typically no more than 1½ inches across.
Field checkCan be scratched with a nail or even swept loose.Cracks are rarely more than 1/8 inch deep.
Structural?Weak surface layer; wears away under traffic.NRMCA says crazing does not affect structural integrity; the main concern is appearance.
When it showsAfter hardening, under traffic.Usually the day after placement or within the first week.

What causes dusting

  • Finishing while bleed water is present, which works water into the top 1/4 inch and makes a weak, high water-cement layer.
  • Broadcasting dry cement or sprinkling water on the surface during finishing.
  • Condensation on cold concrete that is then troweled in, or fresh concrete damaged by rain, snow, drying wind or freezing.
  • Carbon dioxide from unvented heaters, generators and gasoline engines, which can carbonate the surface and reduce its hardness.
  • Insufficient curing, which leaves a soft skin that dusts under foot traffic.
  • Placing directly on polyethylene vapor retarders or non-absorptive subgrades.

What causes crazing

NRMCA says crazing is caused by shrinkage of the paste-rich or mortar-rich surface layer. The same habits that cause dusting feed it: adding water to raise slump, overworking the surface with jitterbugs, vibrating screeds or bull floats, finishing before bleeding ends, spraying water or sprinkling cement to ease finishing, and curing late or not at all. Fast evaporation in low humidity, high temperature, direct sun or wind makes it worse. Crazing is more noticeable on steel-troweled surfaces and shows more as the surface dries after being wet.

Prevention that applies to both

  • Keep slump moderate: 3 to 5 inches. NRMCA says higher slump is acceptable only if the mix reaches it without excess water, for example with water reducers.
  • Do not finish while bleed water is on the surface. Remove it by dragging a garden hose across the surface rather than working it in.
  • Never sprinkle dry cement onto plastic concrete or spray water to ease finishing.
  • Place concrete on 3 to 4 inches of compactible granular fill so some water is absorbed; dampen an absorptive base only when evaporation is high, without letting water pond.
  • Start curing as soon as finishing is done: a liquid membrane curing compound, wet burlap kept continuously moist for at least 3 days, or ponded water. Avoid alternate wetting and drying at an early age.

Can it be repaired?

For dusting, NRMCA describes removing the weak layer by sandblasting, shot blasting or high-pressure washing, then applying a commercial chemical floor hardener such as sodium silicate, zinc fluosilicate or magnesium fluosilicate on thoroughly dried concrete, following the manufacturer’s directions. Severe cases may need wet grinding to sound concrete and a bonded topping. The NRMCA crazing sheet gives no repair methods. For the bigger picture on cracks, see cracks in new concrete, and for freeze-thaw flaking see concrete spalling and scaling.

Sources

Related

Finishing concrete flatwork · Blisters and delamination · All concrete guides

Get a quote

FAQ

Is concrete crazing a structural problem?

NRMCA says crazing does not affect structural integrity and is generally not a precursor to deterioration. The main concern is appearance.

Why is my new concrete powdery?

Common causes per NRMCA are finishing while bleed water is present, sprinkling water or cement on the surface, insufficient curing and carbon dioxide from unvented heaters.

How deep are craze cracks?

NRMCA says they are rarely more than 1/8 inch deep.

How can dusting be prevented?

Use the lowest water content that gives adequate slump, do not finish until bleeding stops, and start curing right after finishing, per NRMCA.

Planning information only, not engineering advice. Surface problems have several possible causes; have a qualified professional evaluate a specific slab. Sources checked Nov 23, 2026.